incorporation of solid particles                

 

 

 

 

new - Bornitrid incorporation - look down

Ni-P-SiC Ni-P-B4C Ni-P-Diamond Ni-P-PTFE
incorporation rate (%) 10 - 25 10 - 33 10 - 25 10 - 25
grain size (µm) 0,5 - 3 0,5 - 3 0,5 - 3 0,2 - 0,5
hardness like deposited 0,1HV 600 +/- 50 600 +/- 50 600 +/- 50 300 +/- 50
hardness after heat treatment  0,1 HV  1200 +/- 100 1200 +/- 100 1300 +/- 100 400 +/- 100
density (g/ml)  6,7 6,6 6,9 6,5
en with 20 % PTFE 

 

 

to connections

to the main page

                                  

new - Bornitrid incorporation in en-coatings  

 

 

 

                                                               

 

 

 

 

                                                         

 

 

 

 

 

boron carbide

ptfe

diamond

silicon carbide

dispersion